A drawing that says ±0.1 mm on a bent, welded, powder-coated bracket is asking four processes to each hold a quarter of the band. That is achievable — but only if you know which step eats what, and in which order.
Step one: the laser
A fibre laser on 1.5 mm mild steel holds cut position to about ±0.05 mm and hole diameter to ±0.1 mm, with a kerf near 0.2 mm. Holes smaller than the sheet thickness cut with visible taper, so a 1 mm hole in 2 mm steel is a drilling job, not a laser one. Grain direction matters too: a long slot cut across the rolling direction will bow after cutting even when the laser did nothing wrong.
Step two: the bend
Air bending holds angle to ±0.3–0.5° and the bend line to ±0.1 mm, but the inside radius follows the die opening — roughly 0.16 × V for mild steel. Bend allowance uses a K-factor near 0.45 for air bending; assume 0.33 and every flange on the part comes up short. The practical rule: keep holes at least 2.5 × thickness away from the bend line, or they pull into ovals.
Step three: welding
TIG on 2 mm stainless pulls 0.5–1.5 mm of distortion per metre of seam unless the sequence is planned. On visible parts we weld in short runs, alternate sides, and let the part cool between passes. Where the design allows it, a tab-and-slot joint or a rivet removes the distortion entirely.
Step four: the finish
Powder coating adds 60–80 µm per side. On a 5 mm slot that is 12–16% of the opening — enough to stop a 5 mm insert. Anodising grows the surface by roughly half the oxide thickness and shifts colour with alloy: 6061 and 5052 will not match after the same bath, however carefully both are racked.
How the stack is managed
We hold the flat pattern to ±0.05 mm, the bend to ±0.3°, and inspect the first article on the CMM with the part clamped in its assembly position rather than lying free on a table. In-process checks run every two hours on bend angle and hole position; outgoing inspection is 100% on fit-critical dimensions.
For assemblies the design lever is adjustment, not precision: slots instead of round holes, self-locating tabs, and one face left unpainted to serve as a datum.
What to send with the RFQ
A DXF or STEP of the flat pattern if you have one, the bend lines, the finish, and the assembly the part has to fit into. If the fit is the real requirement, say so — we will hold the assembly and let the individual part move inside its own tolerance, which is usually cheaper than tightening the drawing.